Prepare the joint, set the machine, strike the arc and travel at the right speed: the basics of stick welding and the faults to avoid.

In stick (MMA) welding, the arc melts both the steel and the coated electrode. The coating shields the weld pool.
Clean off rust, paint and grease, including where the ground clamp sits. Bevel plate thicker than about 5 mm. As a rule of thumb use 30 to 40 A per millimetre of electrode diameter, then follow the figures on the box.
Strike like a match and keep a short arc. In the flat position tilt the electrode 10 to 20 degrees and drag it. For vertical-up, lower the current by about 10 to 15 % and pause briefly on each edge. Chip and brush between passes.
| Fault | Likely cause |
|---|---|
| Electrode sticks | Current too low |
| Burn-through | Current too high or travel too slow |
| Porosity | Damp electrode, dirty metal or long arc |
| Undercut | Current too high or travel too fast |
You will need E6013 or E7018 electrodes, an electrode holder, a ground clamp and eye protection.